Ferrite | Br (Gauss) | Hc (Oe) | Hci (Oe) | (BH)max (MGOe) | Reversible Temperature Coefficients Br%/°C | Reversible Temperature Coefficients Hcj%/°C | Continuous Working Temp. Max °C | BH Curve |
C0 | 2,100 – 2,300 | 1,600 – 2,000 | 2,650 – 2,950 | 0.7 – 1.1 | -0.20 | 0.35 | 350 | |
C1 | 2,250 – 2,450 | 1,750 – 2,050 | 3,100 – 3,400 | 0.9 – 2.0 | -0.20 | 0.35 | 350 | |
C4 | 3,200 – 3,400 | 1,700 – 2,100 | 1,750 – 2,150 | 2.3 – 2.7 | -0.20 | 0.35 | 350 | |
C4B | 3,800 – 4,000 | 1,800 – 2,200 | 1,850 – 2,250 | 3.0 – 3.4 | -0.20 | 0.35 | 350 | |
C5 | 3,800 – 4,050 | 2,200 – 2,600 | 2,250 – 2,650 | 3.2 – 3.6 | -0.20 | 0.35 | 350 | BH Curve |
C7 | 3,700 – 3,900 | 3,300 – 3,650 | 3,850 – 4,150 | 3.6 – 3.8 | -0.20 | 0.35 | 350 | BH Curve |
C8 | 3,900 – 4,100 | 3,000 – 3,400 | 3,050 – 3,450 | 3.4 – 3.8 | -0.20 | 0.35 | 350 | BH Curve |
C8H | 3,700 – 3,900 | 3,500 – 3,800 | 4,800 – 5,100 | 3.2 – 3.6 | -0.20 | 0.35 | 350 | |
C8B | 3,950 – 4,150 | 3,300 – 3,650 | 3,500 – 3,800 | 3.6 – 4.0 | -0.20 | 0.35 | 350 | |
C9H | 3,900 – 4,100 | 3,670 – 3,970 | 4350 – 4650 | 4.0 – 4.4 | -0.20 | 0.35 | 350 | |
C9B | 4,300 – 4,500 | 3,100 – 3,400 | 3,150 – 3,450 | 4.4 – 4.8 | -0.20 | 0.35 | 350 | |
C10 | 4,000 – 4,200 | 2,700- 3,000 | 2,750 – 3,050 | 3.7 – 4.1 | -0.20 | 0.35 | 350 | |
C10H | 4,100 – 4,300 | 3,550 – 3,850 | 3,850 – 4,150 | 4.0 – 4.4 | -0.20 | 0.35 | 350 | |
C11 | 4,200 – 4,400 | 4,020 – 4,320 | 4,850 – 5.150 | 4.2 – 4.6 | -0.20 | 0.35 | 350 | |
C12 | 4,500 – 4,700 | 3,200 – 3,500 | 3,450 – 3,750 | 4.8 – 5.2 | -0.20 | 0.35 | 350 |